Are there any (Australian??) distributors/suppliers for CR1, or is it a
case of contact Baikowski direct?

Matthew

On Wed, 15 Nov 2023 at 16:55, Reinhard Kleeberg <
kleeb...@mineral.tu-freiberg.de> wrote:

> If CR1 is added as internal standard (20 mass%) to rock samples prior
> to McCrone milling and flat powder samples for Bragg-Brentano are
> carefully prepared, we did not observe severe preferred orientation
> for the corundum, maybe as the powder is fine enough
> (particles/aggregates ~ 1 µm before milling) to be randomly
> distributed in the mixture within the gaps between the coarser mineral
> grains.
> But as Jim mentioned, the profile shape of CR1 is suboptimal, we need
> a bimodal crystallite size distribution model to fit. Anyway, for
> routine QPA the material is working.
> Best regards
>
> Reinhard
>
> Zitat von Daniel Chateigner 20210513 <daniel.chateig...@ensicaen.fr>:
>
> > and not textured ?
> >
> > Le 14/11/2023 à 12:56, Reinhard Kleeberg a écrit :
> >> Hi Jim,
> >> great news, would be good to have a corundum what can be modelled
> >> with an easier profile shape model.
> >> Best regards
> >>
> >> Reinhard
> >>
> >> Zitat von "Cline, James P. Dr. (Fed)" <james.cl...@nist.gov>:
> >>
> >>> Hi all,
> >>>
> >>> SRM 676a consisted of Baikowski CR1.  This material is of a
> >>> non-ideal crystallite size distribution: quite broad with tales to
> >>> large crystallites.  SRM 676b was custom made for us by Baikowski
> >>> with a more uniform crystallite size distribution in the 200 nm
> >>> region.  We are working on the certification, rather complex, see:
> >>> doi:10.1107/S0108767311014565 .  It seems that modern beamlines
> >>> don't favor the large specimen size needed for our experiments.
> >>> We have good data from one source, we are looking for some from
> >>> another as we like to see results from more one machine.
> >>>
> >>> Jim
> >>>
> >>>
> >>> James P. Cline
> >>> Materials Measurement Science Division
> >>> National Institute of Standards and Technology
> >>> 100 Bureau Dr. stop 8370 [ B113 / Bldg 217 ]
> >>> Gaithersburg, MD 20899-8523    USA
> >>> james.cl...@nist.gov
> >>> https://www.nist.gov/people/james-p-cline (301) 975 5793
> >>>
> >>> -----Original Message-----
> >>> From: rietveld_l-requ...@ill.fr <rietveld_l-requ...@ill.fr> On
> >>> Behalf Of Reinhard Kleeberg
> >>> Sent: Monday, November 13, 2023 1:51 AM
> >>> To: rietveld_l@ill.fr
> >>> Subject: Re: NIST-676a
> >>>
> >>> We are using Baikowski CR1
> >>> https://www.baikowski.com/en/serie/cr/ Not certified but maybe
> >>> identical with SRM676a. Scale factors and cell parameters found to
> >>> be within the errors. Profile shape shows similar features (also
> >>> not an ideal material).
> >>> Best regards
> >>> Reinhard
> >>>
> >>>
> >>> Zitat von Matthew Rowles <rowle...@gmail.com>:
> >>>
> >>>> Hi Matej
> >>>>
> >>>> You can try IMS135 - high purity alumina.
> >>>>
> >>>> https://imst/
> >>>> andards.com.au%2Fproducts%2F&data=05%7C01%7Cjames.cline%40nist.gov
> %7C2
> >>>> d945a33db074232a69808dbe414ca9a%7C2ab5d82fd8fa4797a93e054655c61dec%7C1
> >>>> %7C0%7C638354550207433666%7CUnknown%7CTWFpbGZsb3d8eyJWIjoiMC4wLjAwMDAi
> >>>> LCJQIjoiV2luMzIiLCJBTiI6Ik1haWwiLCJXVCI6Mn0%3D%7C3000%7C%7C%7C&sdata=r
> >>>> MK%2BzDuAMv2q7U6fCpu38mzuqIrTdCiQfNDPSmB%2BQZk%3D&reserved=0
> >>>>
> >>>> It was certified against some SRM676a we already had in the lab.
> >>>>
> >>>>
> >>>> Matthew
> >>>>
> >>>>
> >>>>
> >>>>
> >>>> On Sun, 12 Nov 2023 at 22:42, Matej Dolenec <smu...@siol.net> wrote:
> >>>>
> >>>>> Dear all,
> >>>>>
> >>>>> I am trying to buy NIST-676a but unfortunately unsuccessful ... I was
> >>>>> trying to find it on NIST, ALDRICH and other sites but the standard
> >>>>> is out of stock. Does anybody has any information if this standard
> >>>>> will be available soon and where? If not, which standard should I use
> >>>>> instead of NIST-676a? I was using this standard for amorphous
> >>>>> phase identification.
> >>>>>
> >>>>> Regrads, Matej
> >>>>>
> >>>>> ++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
> >>>>> Please do NOT attach files to the whole list
> >>>>> <alan.he...@neutronoptics.com
> >>>>>>
> >>>>> Send commands to <lists...@ill.fr> eg: HELP as the subject with no
> >>>>> body text The Rietveld_L list archive is on
> >>>>> http://www/.
> >>>>> mail-archive.com%2Frietveld_l%40ill.fr
> %2F&data=05%7C01%7Cjames.cline%
> >>>>> 40nist.gov
> %7C2d945a33db074232a69808dbe414ca9a%7C2ab5d82fd8fa4797a93e0
> >>>>> 54655c61dec%7C1%7C0%7C638354550207433666%7CUnknown%7CTWFpbGZsb3d8eyJW
> >>>>> IjoiMC4wLjAwMDAiLCJQIjoiV2luMzIiLCJBTiI6Ik1haWwiLCJXVCI6Mn0%3D%7C3000
> >>>>> %7C%7C%7C&sdata=nnVgkFx8mHZ%2Br%2Bng9oJ00Uz9wBy9MYDZ%2F46l%2F3%2BUGg8
> >>>>> %3D&reserved=0
> >>>>> ++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
> >>>>>
> >>>>>
> >>>
> >>>
> >>> --
> >>> TU Bergakademie Freiberg
> >>> Dr. R. Kleeberg
> >>> Mineralogisches Labor
> >>> Brennhausgasse 14
> >>> D-09596 Freiberg
> >>>
> >>> Tel. ++49 (0) 3731-39-3244
> >>> Fax. ++49 (0) 3731-39-3129
> >>
> >>
> >>
> >> ++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
> >> Please do NOT attach files to the whole list
> <alan.he...@neutronoptics.com>
> >> Send commands to <lists...@ill.fr> eg: HELP as the subject with no
> body text
> >> The Rietveld_L list archive is on
> >> http://www.mail-archive.com/rietveld_l@ill.fr/
> >> ++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
> >>
> > --
> >
> > ----------------------------------------------------------------------
> > Daniel Chateigner
> > Professeur Normandie Universite
> > http://www.ecole.ensicaen.fr/~chateign/danielc/
> > ----------------------------------------------------------------------
> > Editor: "Combined Analysis", Wiley-ISTE:
> > http://eu.wiley.com/WileyCDA/WileyTitle/productCd-1848211988.html
> > Workshops on Combined Analysis:
> > http://www.ecole.ensicaen.fr/~chateign/formation/
> > ----------------------------------------------------------------------
> > Address:
> > CRISMAT-ENSICAEN and IUT-Caen,
> > Universite de Caen Normandie, campus 2
> > 6, Bd. M. Juin 14050 Caen, France
> > tel: 33 (0)2 31 45 26 11
> > daniel.chateig...@ensicaen.fr
> > ----------------------------------------------------------------------
> > Open Databases:
> > Material Properties Open Database (MPOD): mpod.cimav.edu.mx
> > Crystallography Open Database     (COD):
> http://www.crystallography.net/cod/
> >                   Theoretical     (TCOD):
> > http://www.crystallography.net/tcod/
> >                   Predicted       (PCOD):
> > http://www.crystallography.net/pcod/
> > Raman Open Database (ROD): solsa.crystallography.net/rod/
> > Full-Profile Search-Match (FPSM): cod.iutcaen.unicaen.fr/
> > ----------------------------------------------------------------------
>
>
> --
> TU Bergakademie Freiberg
> Dr. R. Kleeberg
> Mineralogisches Labor
> Brennhausgasse 14
> D-09596 Freiberg
>
> Tel. ++49 (0) 3731-39-3244
> Fax. ++49 (0) 3731-39-3129
>
> ++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
> Please do NOT attach files to the whole list <alan.he...@neutronoptics.com
> >
> Send commands to <lists...@ill.fr> eg: HELP as the subject with no body
> text
> The Rietveld_L list archive is on
> http://www.mail-archive.com/rietveld_l@ill.fr/
> ++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
>
>
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to