You should make a first refinement with ATZ=0 for both phases, and let the 
value that the software has calculated. 
Be carefull, the first atom site must be fully occupied.
Patrick
      De : Kotaro SAITO <kotaro.sa...@kek.jp>
 À : Rietveld_l@ill.fr 
 Envoyé le : Mardi 24 février 2015 11h52
 Objet : Quantitative phase analysis on FullProf
   
Dear Rietvelders,

Does anyone know how FullProf calculates weight fractions “Fract(%)” in a .sum 
file? or Is there any known bugs for calculating ATZ?

According to the manual, it seems that ATZ is used for calculating the 
values... but no further information is written in the manual.
I am also wondering, in my case, why different phases have the exact same value 
for ATZ. It should be different for different materials from the definition in 
the manual.
Here are the related descriptions in my .out file.
    Phase 1
    => The given value of ATZ is        688.48 the program has calculated:      
  4345.96
    Phase 2
    => The given value of ATZ is        688.48 the program has calculated:      
  576.91
I confirmed that 4345.96 and 576.91 seem to be Z*Mw

I calculated the weight fractions using the values in the sum file and a 
equation Wp=S_p(ZMV)_p/ΣS_i(ZMV)_i (R. J. Hill and C. J. Howard, J Appl. 
Cryst., 20, 467-474), and ended up in getting quite different fractions from 
those in the .sum file. I got 97.3% and 2.7% with my calculation and the values 
in the .sum file are like this.
    Phase 1
    => Bragg R-factor:  2.74      Vol:  941.374( 0.009)  Fract(%):  82.46( 0.85)
    => Rf-factor=  1.81            ATZ:        688.475  Brindley:  1.0000
    Phase 2
    => Bragg R-factor:  7.65      Vol:  137.093( 0.079)  Fract(%):  17.54( 0.97)
    => Rf-factor=  5.35            ATZ:        688.475  Brindley:  1.0000


When I ran an example pcr for quantitative phase analysis in Examples 
(si3n4r.pcr), I got ATZ and weight fractions below
Si3N4 alpha
 => The given value of ATZ is        560.00 the program has calculated:        
561.14
Si3N4 beta
 => The given value of ATZ is        280.00 the program has calculated:        
280.57

 => Phase:  1      Si3 N4 alpha
 => Bragg R-factor:  0.969      Vol:  292.623( 0.016)  Fract(%):  92.88( 0.44)
 => Rf-factor= 0.600            ATZ:        560.000  Brindley:  1.0000

 => Phase:  2      Si3 N4 beta
 => Bragg R-factor:  2.26      Vol:  145.711( 0.027)  Fract(%):    7.12( 0.09)
 => Rf-factor=  1.09            ATZ:        280.000  Brindley:  1.0000

and the these fractions are consistent with those derived from the equation 
Wp=S_p(ZMV)_p/ΣS_i(ZMV)_i.

I would like to know which weight fractions I should trust for my case…

Best regards,

Kotaro

//================//================//
  Kotaro SAITO
  High Energy Accelerator Research Organization
  Institute of Materials Structure Science
  1-1 Oho, Tsukuba, Ibaraki, 305-0801, Japan
//================//================//

++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++


  
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to