Hi Claire
It sounds like you're using the Hill/Howard algorithm for quantification.
You just need to not put the details of the SiO2 phase you're using into
the summation.
This is equivalent to removing the ~90% attributed to the capillary, and
renormalising to 100%
Matthew
On Tue, 14 Nov 20
Il 13/11/2023 18:35, Claire Emily Boronski ha scritto:
Dear Claire,
Make the sum of the remaining crystalline weight percentages to be 100%.
This is a rough, but simple, calculation.
Alternatively, measure an empty capillary and correct the raw data of
your mixture for such scattering (taking
Hi All,
I am trying to exclude the glass capillary from the weight percent calculations
in my Rietveld refinement. I modeled the glass capillary using a SiO2 CIF file
and made the crystallite size very small. The issue I am having now is that in
the weight percent calculation it is saying the g