Low temperature x-ray diffraction on Powdered single crystals was taken from 5 
to 80 degree with step size 0.02. The intensity of strongest peak is around 
10000. Space group is Bb21m.

The zero shift is quite large for both methods refinements. In GSAS, it is 
around -30.

发件人: [email protected] [mailto:[email protected]] 代表 Lucas 
Bonan Gomes
发送时间: 2016年6月15日 0:47
收件人: [email protected]
主题: Re: Le bail and rietveld method


Dear Jin,

Tell us about the parameters used in the analysis, such as step size.

Lucas Bonan Gomes.
Em 14/06/2016 13:32, Peng, Jin escreveu:
Dear Collegues:

I am recently working on the structure refinement of some inorganic single 
crystals. I got the structure parameters from two ways:

1.       Single crystal x-ray refinement;

2.       Low temperature x-ray diffraction on Powdered single crystals.
I refined the powder x-ray diffraction pattern with both rietveld method and Le 
bail method. However, the Le bail refinement result is consistent with single 
crystal x-ray while the rietveld show divergence. Both a, b, c are remarkably 
high than other two method. For example, c is 19.573 for single crystal xrd and 
19.576 for le bail method. While for rietveld, it is 19.62.

The powder x-ray pattern are taken from cuprate sample holder. I noticed that 
its peak position is around 0.15 degree lower (2theta) than the spectrum taken 
at glass sample holder.

Jin




++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Please do NOT attach files to the whole list 
<[email protected]><mailto:[email protected]>

Send commands to <[email protected]><mailto:[email protected]> eg: HELP as the 
subject with no body text

The Rietveld_L list archive is on http://www.mail-archive.com/[email protected]/

++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++



++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <[email protected]>
Send commands to <[email protected]> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/[email protected]/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to