Well,
I do not work with metals and therefore my question could be somehow naive. Suppose you have such funny peaks and you are sure it is not due to experimental conditions. How unique is than the interpretation offered by Leonid ? Nothing presonal, of course :-)
lubo




On Mon, 15 Jun 2015, Leonid Solovyov wrote:

Dear Apu,

As the 2nd peak seems to be broader than the 1st one, the broadening is most 
probably due to the stacking faults, typical for the close-packed metals. The 
asymmetry and complexity of the broadening might also suggest the presence of 
crystallites with different degree of faulting (and/or size). Among DDM ( 
http://sites.google.com/site/ddmsuite ) examples there is a model for Cu ( 
\DDM195d\EXAMPLES\Defects\Cu.ddm ), accounting for the influence of faults on 
both peak broadening and intensities. It may also be applicable to Ni, but in 
this particular case a two-phase model might be necessary to allow for the 
presence of different crystalline fractions.

Best regards,
Leonid

*******************************************************
Leonid A. Solovyov
Institute of Chemistry and Chemical Technology
660036, Akademgorodok 50/24, Krasnoyarsk, Russia
http://sites.google.com/site/solovyovleonid
*******************************************************


________________________________
From: Apu Sarkar <apusar...@gmail.com>
To: "rietveld_l@ill.fr" <rietveld_l@ill.fr>
Sent: Monday, June 15, 2015 12:59 PM
Subject: Peak assymtery not able to fit



Hi,

I am working on a nanocrystalline Nickel sample. I am not able to fit the peaks 
to get FWHM and Integral Breadth.

Please see the attached images. Fig. 1 shows the profile and a zoomed view of a 
peak. Tail part of the peak is broader.

Fig. 2 shows the winplotr fit. It is not matching the max intensity.

Please give you suggestions to get a better fit for this kind of XRD peak.


Thanks
Apu

++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <alan.he...@neutronoptics.com>
Send commands to <lists...@ill.fr> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/rietveld_l@ill.fr/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to