COL ICSD Collection Code 14383
DATE Recorded Jan 1, 1980; updated Nov 3, 1987
NAME Strontium tecto-heptaoxotetraborate
FORM Sr B4 O7
= B4 O7 Sr
TITL The Crystal Structure of the Strontium and Lead
Tetraborates, Sr O
(B2 O3)2 and Pb O (B2 O3)2
REF Acta Crystallographica (1,1948-23,1967)
ACCRA 20 (1966) 274-279
AUT Perloff A, BlockÿS
CELL a=4.237(4) b=4.431(4) c=10.706(10) à=90.0
á=90.0 ç=90.0
V=201.0 Z=2
SGR P 21 n m (31) - orthorhombic
CLAS mm2 (Hermann-Mauguin) - C2v (Schoenflies)
PRS oP24
ANX AB4X7
PARM Atom__No OxStat Wyck -----X----- -----Y-----
-----Z----- -SOF-
Sr 1 2.000 2a 0. 0.2119(3) 0.
O 1 -2.000 2a 0.585(5) 0.772(3) 0.
O 2 -2.000 4b 0.547(4) 0.357(2)
0.141(1)
O 3 -2.000 4b 0.144(4) 0.725(2)
0.135(1)
O 4 -2.000 4b 0.147(3) 0.132(2)
0.277(1)
B 1 3.000 4b -0.041(9) 0.327(3)
0.378(1)
B 2 3.000 4b -0.006(12) 0.823(3)
0.248(1)
WYCK b5 a2
ITF Sr 1 B=0.41
ITF O 1 B=0.75
ITF O 2 B=0.63
ITF O 3 B=0.7
ITF O 4 B=0.53
ITF B 1 B=0.68
ITF B 2 B=0.76
RVAL 0.071
--------------------------------------------------------------------------------
----- Original Message Follows -----
From: Renato Bastos Guimarães <[EMAIL PROTECTED]>
To: "RIETVELD_L Distribution List" <[email protected]>
Date: Tue, 6 Jun 2006 18:35:57 -0300
> Dear all!!
>
> Can someone send me the structure of SrB4O7?
> It is not at the free database.
>
> Thank you
>
> Renato Bastos Guimarães.
> Instituto de Física
> Universidade Federal Fluminense
> Laboratório de Difração de Raios X-uff
Marco Sommariva
----------------------------------------------------------
Marco Sommariva
Department of Materials Science
University Milano-Bicocca
Via R. Cozzi 53, 20125 Milano (ITALY)
mail: [EMAIL PROTECTED]
phone: 0039.02.64.48.51.41
fax: 0039.02.64.48.54.00
----------------------------------------------------------